Activated carbon adsorbs dissolved gold on the surface of its pore structure, and that structure becomes fouled in service. Lime and hard water deposit scale, while oils, reagents and natural organic matter from the ore coat the surfaces. Fouled carbon adsorbs gold more slowly, so more gold leaves in the tailings solution. Regeneration restores the carbon: an acid wash with hydrochloric acid dissolves the scale, and heating in a kiln in steam removes the organic matter and reopens the pores, after which the carbon is returned to the circuit.
This article covers the regeneration steps, the kiln duty and the measurement of regeneration performance. The measurement of carbon activity is described in activated carbon testing, and elution in carbon elution.
Carbon foulants
| Foulant | Source | Removed by |
|---|---|---|
| Calcium carbonate and other scale | Lime, hard process water | Hydrochloric acid wash |
| Silica, other inorganic precipitates | Ore and water chemistry | Partly by acid wash; some build up permanently |
| Flotation reagents, oils, greases | Upstream flotation, equipment | Thermal reactivation |
| Humic and other natural organics | Ore, water | Thermal reactivation |
Thermal reactivation
Wet, drained carbon is fed to a kiln, usually a rotary kiln, although vertical kilns are also used. The first section dries the carbon, and the moisture it carries provides steam. In the hot zone, organic material is pyrolysed and the carbon is reactivated in a steam atmosphere at around 650 °C. Temperature is critical: if it is too low or the residence time too short, the organics are not removed, while very high temperatures in the absence of oxygen can graphitise the pyrolysis residue and reduce activity. The hot carbon is quenched in water, screened to remove fines and returned to the circuit.
where
- kiln feed rate (kg/h, dry basis)
- residence time of carbon in the hot zone (h)
- ,
- adsorption rate constants from the same carbon activity test
Worked example: the CIL circuit elutes 4.3 t of carbon per day. To regenerate all of it in 20 kiln hours per day, the kiln must process 4,300 ÷ 20 = 215 kg/h of dry carbon. Kiln capacity is quoted on a dry basis, but the kiln must also evaporate the water carried in with the drained carbon, which accounts for a large share of its heat duty. Residence time in the hot zone is determined by the kiln design, speed and slope, and is checked against the supplier's rating.
Measuring regeneration performance
Carbon samples taken before and after the kiln, together with a sample of new carbon, are tested by the same activity method. The activity ratio shows the proportion of the original adsorption rate recovered by the regenerated carbon. Published experience suggests that many plants regenerate poorly, at well under half the activity of new carbon, while good practice achieves more than 70%. A declining ratio over time points to problems with kiln temperature, residence time or steam, or to a foulant that the acid wash is not removing.
Carbon losses
where
- carbon lost per tonne of ore (g/t)
- fresh carbon added over the period (g)
- change in carbon held in the circuit, from tank carbon concentration surveys (g)
- tonnes of ore treated over the period (t)
Worked example: during a month the plant adds 2.5 t of new carbon, and the carbon inventory surveys show the circuit holding 0.3 t more than at the start of the month. Over 216,000 t of ore, the carbon loss is (2.5 − 0.3) × 1,000,000 ÷ 216,000 = 10.2 g/t.
Carbon fines carry loaded gold, so lost carbon also represents lost gold. Fines from the sizing screen and the safety screens should be collected and treated, and increasing losses investigated, with worn interstage screens, high agitator speeds and attrition in pumps and the kiln as the usual causes.
Glossary
- Activated carbon
- Carbon with a very large internal surface area that adsorbs gold cyanide.
- Fouling
- Build-up of scale or organic matter that blocks carbon pores.
- Acid wash
- Washing carbon with dilute hydrochloric acid to dissolve carbonate and other scale.
- Thermal reactivation
- Heating carbon in steam in a kiln to remove organic fouling and restore pores.
- Activity ratio
- Adsorption rate of regenerated carbon divided by that of new carbon, from the same test.
- Quench
- Rapid cooling of hot carbon in water as it leaves the kiln.
- Carbon fines
- Small carbon particles broken from granules; they carry gold and are lost from the circuit if not captured.
- Carbon inventory
- The mass of carbon held in the adsorption circuit.
Frequently asked questions
Why is carbon regenerated?
Because fouled carbon adsorbs gold more slowly, so more gold is lost in the tailings solution and more carbon is required in the circuit.
At what temperature does a carbon kiln operate?
Thermal reactivation is commonly described at around 650 °C in steam. The supplier's rating and plant activity tests determine the actual setpoint.
Should acid washing be carried out before or after elution?
Either sequence can work. Plants choose according to their chemistry and equipment; the aim is to remove carbonates before they block the pores.
How can kiln performance be confirmed?
Run the same activity test on new carbon, on carbon entering the kiln and on carbon leaving it, and track the activity ratio over time.
Discuss your plant with a metallurgist
Tiegel is a Perth metallurgy company. We help with testwork, plant optimisation, metal accounting and investigations, and we build the Tiegel Suite software.
Talk to a metallurgistReferences and further reading
- Marsden, J.O. and House, C.I. (2006). The Chemistry of Gold Extraction, 2nd edition. Society for Mining, Metallurgy and Exploration.
- 911 Metallurgist. Carbon regeneration. Link
Worked examples and charts marked illustrative use invented figures, not data from any operation.