Tiegel home Talk to a metallurgist

Oxygen uptake testing: measuring the oxygen demand of leach slurry

Measuring the oxygen uptake rate of a leach slurry, converting it to oxygen demand per tonne, and using it to size aeration or pre-oxidation.

· 4 minute read · By

Gold cyanidation requires oxygen, and some ores, particularly those containing pyrrhotite, contain minerals that also consume oxygen. Where these minerals consume oxygen faster than sparging can supply it, dissolved oxygen in the leach tanks falls and gold dissolution slows. The oxygen uptake rate (OUR) test measures this demand directly: a slurry sample is saturated with oxygen, the gas supply is stopped, and the rate at which dissolved oxygen falls is recorded. The test is quick, inexpensive and particularly useful for plants treating sulphide ores. This article gives the procedure, the calculation and the application of the result. Our article on dissolved oxygen in cyanide leaching explains the role of oxygen in the leach.

Oxygen uptake test stepsTake fresh slurry, sparge to high dissolved oxygen, stop sparging and stir gently, log dissolved oxygen against time, take the slope.Fresh slurryplant densitySparge withair or O₂Stop gas,stir gentlyLog DOevery 30 sSlope =uptake raterun at plant temperature, pH and cyanide strength; test within minutes of sampling
The oxygen uptake test. Fresh samples matter: sulphides keep reacting in the sample bucket and the rate falls with time.

Test procedure

  1. Sample fresh slurry from the leach feed or a leach tank and test it within minutes.
  2. Hold the temperature, pH and cyanide at plant values, and mix gently enough to keep the solids suspended without entraining air.
  3. Sparge air or oxygen to raise the dissolved oxygen well above the plant operating level.
  4. Stop the gas and record dissolved oxygen every 30 seconds for several minutes with a calibrated probe.
  5. Fit a straight line to the falling section, the slope of which is the uptake rate, and repeat on duplicate samples.

Calculation

OUR=−dDOdtO₂ demand=OUR×vslurry×60

where

OUR
oxygen uptake rate: the slope of dissolved oxygen against time (mg/L per minute)
vslurry
slurry volume per tonne of dry solids (m³/t); 1 mg/L is 1 g/m³
O₂ demand
oxygen consumed per tonne of solids per hour (g/t·h)

Worked example: dissolved oxygen falls from 18.0 to 17.29 mg/L in six minutes, and the fitted slope is 0.119 mg/L per minute. The slurry is 45% solids with a solids SG of 2.7, so each tonne of solids is contained in 1/2.7 + 0.55/0.45 = 1.59 m³ of slurry.

Oxygen demand = 0.119 g/m³·min × 1.59 m³/t × 60 = 11.4 g of oxygen per tonne per hour. At 300 t/h, the first leach tank must supply about 3.4 kg of dissolved oxygen per hour to meet the demand of the ore alone, before any oxygen is available for gold dissolution.

Dissolved oxygen falling after aeration stopsDissolved oxygen falls from 18.0 to 17.3 mg/L in six minutes in the as-received slurry, and only to 17.8 mg/L after pre-aeration.17.017.417.818.20123456Time after aeration stopped (min)Dissolved oxygen (mg/L)As receivedAfter pre-aerationAs received: 0 → 18.0As received: 1 → 17.9As received: 2 → 17.8As received: 3 → 17.6As received: 4 → 17.5As received: 5 → 17.4As received: 6 → 17.3As received: 0.12After pre-aeration: 0 → 18.0After pre-aeration: 1 → 18.0After pre-aeration: 2 → 17.9After pre-aeration: 3 → 17.9After pre-aeration: 4 → 17.8After pre-aeration: 5 → 17.8After pre-aeration: 6 → 17.8Pre-aerated: 0.04
Oxygen uptake test. The slope of each line is the oxygen uptake rate. Pre-aeration oxidised the most reactive sulphides and cut the rate to a third. Illustrative figures.

After 8 hours of pre-aeration, the same slurry consumed oxygen at only 0.04 mg/L per minute, because the most reactive sulphide surfaces had been oxidised (passivated) before cyanide was added.

Application of the result

Oxygen demand per tonne, combined with the transfer efficiency of the sparging system, determines the air or oxygen flow required.

The result also informs the choice between air and oxygen. Air limits dissolved oxygen to about 8 mg/L at 25 °C at sea level, while pure oxygen allows much higher levels, and ores with a high demand often require oxygen or shear reactors to maintain dissolved oxygen.

If uptake falls sharply after aeration, a pre-aeration tank ahead of cyanide addition can reduce both oxygen and cyanide consumption in the leach.

Routine uptake tests on the leach feed also identify new ore types containing reactive sulphides before they affect recovery.

Sources of error

  • Delay between sampling and testing, since uptake falls with every minute the sample stands.
  • An uncalibrated probe or one with a slow response, which flattens the measured slope.
  • Air entering at the surface during logging, which adds oxygen and lowers the measured rate.
  • Test conditions that differ from the plant, since uptake depends on pH, cyanide and lead nitrate additions.

Glossary

Oxygen uptake rate
How fast a slurry consumes dissolved oxygen (mg/L per minute).
Dissolved oxygen
Oxygen gas dissolved in the solution, measured in mg/L.
Pyrrhotite
An iron sulphide mineral that reacts quickly with oxygen and cyanide.
Pre-aeration
Aerating slurry before cyanide is added to oxidise reactive sulphides.
Passivation
Forming a coating on a mineral surface that slows further reaction.
Sparging
Bubbling air or oxygen into a tank.
Shear reactor
A device that dissolves oxygen into slurry under high shear and pressure.

Frequently asked questions

How is the oxygen uptake rate of a slurry measured?

Saturate fresh slurry with oxygen, stop the gas, keep the slurry gently mixed, record dissolved oxygen every 30 seconds, and take the slope of the straight section of the curve.

How is the oxygen uptake rate converted to kilograms per hour?

Multiply the rate in mg/L per minute (equivalent to g/m³ per minute) by the slurry volume per tonne and by 60 to obtain grams per tonne per hour, then multiply by the throughput in tonnes per hour.

What causes high oxygen uptake?

Reactive sulphide minerals, particularly pyrrhotite, and some other minerals and organic matter that consume oxygen.

Does pre-aeration help?

Often. Oxidising the most reactive sulphide surfaces before cyanide addition can reduce oxygen and cyanide consumption in the leach. The effect should be confirmed with uptake measurements before and after pre-aeration.

Discuss your plant with a metallurgist

Tiegel is a Perth metallurgy company. We help with testwork, plant optimisation, metal accounting and investigations, and we build the Tiegel Suite software.

Talk to a metallurgist

References and further reading

  1. Marsden, J.O. and House, C.I. (2006). The Chemistry of Gold Extraction, 2nd edition. Society for Mining, Metallurgy and Exploration.
  2. Rumball, J.A. and Houchin, M.R. (2003). Cyanide: oxygen ratio for leaching gold in sulphide ores. International Mineral Processing Congress.

Worked examples and charts marked illustrative use invented figures, not data from any operation.