Tiegel home Talk to a metallurgist

Copper heap leach, solvent extraction and electrowinning: copper transfer, acid and current

Copper heap leach SX-EW: copper transfer from PLS flow and grades, acid regenerated in electrowinning, cell current and energy per tonne of copper.

· 4 minute read · By

Oxide copper ores, and some sulphide ores, can be treated without grinding or flotation. The ore is stacked on a lined pad and irrigated with dilute sulphuric acid, which dissolves the copper as it percolates through the heap, and the pregnant leach solution (PLS) drains from the base. The PLS is too dilute and too impure for direct electrowinning, so solvent extraction transfers the copper into a clean, concentrated acid electrolyte, from which electrowinning deposits copper cathode for sale.

This article follows the copper through the three steps and sets out the principal balances. SX staging is covered in solvent extraction and McCabe-Thiele diagrams, column testing in heap leach column tests, and Faraday's law in electrowinning.

Copper heap leach, solvent extraction and electrowinningAcid solution percolates through the heap and leaves as pregnant leach solution. Solvent extraction moves the copper into organic and then into a strong acid electrolyte. Electrowinning plates copper cathode and returns the acid. Raffinate goes back to the heap.Heap leach(acid irrigation)SX extractionSX strippingElectrowinningCopper cathodePLSloaded organicstripped organicraffinate (acid) back to the heaprich electrolytelean electrolyte
The heap leach SX-EW loop. Two solution circuits never mix: the leach solution and the electrolyte. The organic carries copper from one to the other.

Copper transfer through SX

copper=QPLS×(CPLS−Craff)acid regenerated=98.0863.55=1.54 kg per kg Cu

where

QPLS
pregnant leach solution flow to SX (m³/h)
CPLS, Craff
copper in PLS and in raffinate (g/L, the same as kg/m³)
acid regenerated
sulphuric acid made in electrowinning for each kilogram of copper plated, returned to the heap in raffinate via the strip circuit

Worked example: 1,000 m³/h of PLS at 3.0 g/L copper leaves SX as raffinate at 0.3 g/L. SX recovers 90% of the copper and transfers 1,000 × (3.0 − 0.3) = 2,700 kg/h, or 64.8 t/d, which is about 23,700 t a year at full availability. At an irrigation rate of 10 L/h per m², a solution flow of 1,000 m³/h requires about 10 ha of heap under leach.

Electrowinning that copper regenerates 64.8 × 1.54 = 100 t/d of sulphuric acid in the electrolyte. The acid returns to the heap through SX stripping and the raffinate, so the fresh acid make-up to the heap is mainly the acid consumed by gangue minerals, measured in column tests as kg/t of ore.

Electrowinning current and energy

Itotal=copper per hour (g/h)1.1855×ηkWh/t=Vcell×10001.1855×η

where

1.1855
grams of copper per ampere-hour at 100% current efficiency, from Faraday’s law
η
current efficiency (fraction)
Itotal
amperes summed over all cells; divide by the rectifier current to get the number of cells in series
Vcell
cell voltage (V)

Worked example: depositing 2,700 kg/h at 92% current efficiency requires 2,700,000 ÷ (1.1855 × 0.92) = 2.48 million amperes summed over all cells. With a 30,000 A rectifier and the cells in series, this corresponds to about 83 cells. At an assumed cell voltage of 2.0 V, the electrical energy is 2.0 × 1,000 ÷ (1.1855 × 0.92) = 1,834 kWh per tonne of copper. Lower current efficiency, caused by short circuits or iron in the electrolyte, increases both the number of cells required and the energy per tonne.

Process monitoring

On the heap, the irrigation rate and coverage, PLS grade and flow, acid consumption, and any ponding or channelling on the heap surface should be monitored. In SX, the main concerns are phase separation, entrainment of organic in the electrolyte or of aqueous in the organic, crud build-up and copper remaining in the raffinate.

In EW, current efficiency, cathode quality (nodules and impurities), short circuits and the iron, manganese and chloride levels in the electrolyte require regular attention. Across the whole circuit, the water and acid balance is affected by evaporation from the heap and ponds, by the bleed streams that control impurity build-up, and by rainfall events.

Glossary

Heap leach
Leaching crushed or run-of-mine ore stacked on a lined pad by irrigating it with solution.
PLS
Pregnant leach solution: the copper-bearing solution draining from the heap.
Raffinate
The solution leaving SX after its copper has been extracted; it returns to the heap.
Solvent extraction (SX)
Transferring copper from the leach solution into an organic phase and then into a strong electrolyte.
Electrolyte
The strong copper and acid solution from which copper is electrowon.
Electrowinning (EW)
Plating metal from solution onto cathodes by passing an electric current.
Current efficiency
The share of current that actually plates copper.
Cathode
The plate on which copper is deposited; also the name of the copper product.

Frequently asked questions

How much copper does an SX plant transfer?

PLS flow × (PLS copper − raffinate copper). For 1,000 m³/h at 3.0 g/L in and 0.3 g/L out, the transfer is 2.7 t/h.

Where does the acid for the heap come from?

Electrowinning regenerates about 1.54 kg of acid per kg of copper deposited, which returns to the heap through SX. Fresh acid mainly replaces the acid consumed by gangue minerals.

How many EW cells are required?

Divide the copper deposited per hour in grams by 1.1855 g/Ah and by the current efficiency, then by the rectifier current. For 2,700 kg/h at 92% and 30,000 A, about 83 cells are required.

Why is current efficiency below 100%?

Part of the current drives side reactions, such as cycling iron between its two oxidation states, and part is lost to short circuits between electrodes.

Discuss your plant with a metallurgist

Tiegel is a Perth metallurgy company. We help with testwork, plant optimisation, metal accounting and investigations, and we build the Tiegel Suite software.

Talk to a metallurgist

References and further reading

  1. Schlesinger, M.E., King, M.J., Sole, K.C. and Davenport, W.G. (2011). Extractive Metallurgy of Copper, 5th edition. Elsevier.
  2. Ritcey, G.M. and Ashbrook, A.W. (1984). Solvent Extraction: Principles and Applications to Process Metallurgy, Part I. Elsevier.

Worked examples and charts marked illustrative use invented figures, not data from any operation.