Pressure oxidation and bio-oxidation of refractory gold: chemistry, oxygen demand and acid

How pressure oxidation and bio-oxidation release gold locked in sulphides: reactions, oxygen and acid per tonne of sulphur, and the extent of sulphide oxidation.

· 5 minute read · By

In refractory ores, gold is locked within sulphide minerals as particles too fine to liberate by grinding, or within the mineral lattice, so much of it remains unleached by direct cyanidation. The sulphides must first be oxidised. Pressure oxidation achieves this with heat, pressure and pure oxygen in an autoclave, and bio-oxidation achieves it more slowly with bacteria that derive energy from oxidising sulphides. In both processes the sulphur is converted to sulphuric acid and the iron to oxides or sulphates, exposing the gold to cyanide.

This article covers the chemistry, the oxygen and acid balances, and the measurement of the extent of oxidation. Roasting, the other main route for refractory gold, is covered in roasting of refractory gold, and the tests that establish whether an ore is refractory in diagnostic leach testing.

Pressure oxidation and bio-oxidation flowsheetsBoth routes take a refractory sulphide concentrate, oxidise the sulphides, wash the acid liquor away in thickeners, neutralise it, and send the oxidised solids to cyanide leaching.Refractorysulphide concentrateAutoclave (POX)190–230 °C, O₂Bio-oxidation tanksabout 40 °C, airWash thickeners(CCD)Solids:neutralise, CILAcid liquor:neutraliseeither route(not both)
Simplified POX and BIOX flowsheets. The oxidation step differs; the washing, neutralisation and leaching that follow are similar. Operating conditions are typical values from vendor literature.

Comparison of POX and BIOX

Pressure oxidation (POX)Bio-oxidation (BIOX)
VesselAutoclave, lined and agitated, in compartmentsOpen aerated stirred tanks
Typical conditionsAbout 190 to 230 °C, oxygen partial pressure about 3 to 7 barAbout 40 °C, air sparged; cooling needed because oxidation releases heat
Residence timeHoursSeveral days
Oxygen sourceOxygen plantAir blowers
FeedConcentrate or whole oreUsually flotation concentrate
Sensitive toCarbonates and chlorides in feed, scaling, basic iron sulphate formationTemperature, pH, nutrient supply, and some dissolved species that inhibit the bacteria

The typical conditions are taken from vendor literature; each plant is designed from its own testwork.

Oxygen and acid balance

Under POX conditions much of the iron reports as hematite and the sulphur as sulphuric acid. The overall reaction for pyrite is:

4FeS2+15O2+8H2O→2Fe2O3+8H2SO4mO2mS=15×32.008×32.06=1.87macidmS=98.0832.06=3.06

where

mO2mS
tonnes of oxygen per tonne of pyrite sulphur fully oxidised
macidmS
tonnes of sulphuric acid formed per tonne of pyrite sulphur when the iron ends as hematite
Per tonne of pyrite sulphur fully oxidised1.87 tonnes of oxygen, 3.06 tonnes of sulphuric acid and 3.12 tonnes of limestone to neutralise that acid, from the reaction stoichiometry.Oxygen neededOxygen needed: 1.871.87Sulphuric acid formedSulphuric acid formed: 3.063.06Limestone to neutralise the acidLimestone to neutralise the acid: 3.123.12Tonnes per tonne of sulphur
Stoichiometric quantities for pyrite oxidised to hematite and sulphuric acid. Plants supply more oxygen than this because not all of it is used, and carbonates in the ore consume some of the acid.

Worked example: 100 t/d of concentrate containing 25% sulphide sulphur, mostly as pyrite, contains 25 t/d of sulphur. Complete oxidation requires 25 × 1.87 = 47 t/d of oxygen by stoichiometry. Not all of the oxygen fed is utilised, so the oxygen plant must be larger; at an assumed utilisation of 85% it must supply about 55 t/d. The oxidation produces about 25 × 3.06 = 76 t/d of sulphuric acid, and neutralising all of it with limestone would require about 78 t/d, less any acid consumed by carbonates in the feed. Arsenopyrite and other sulphides have their own stoichiometry and are added to the balance for actual feeds.

In practice, some iron and sulphate report as basic iron sulphate or jarosite rather than hematite and free acid, which alters the acid balance and can increase lime and cyanide consumption downstream. Testwork quantifies these effects, and some plants hold the autoclave discharge at temperature for a period (hot curing) to redissolve basic iron sulphate before washing.

Measuring sulphide oxidation

sulphide oxidation=Sfeed−Sresidue×MresidueMfeedSfeed×100

where

Sfeed, Sresidue
sulphide sulphur in the feed and in the oxidised residue (%)
MresidueMfeed
residue mass per unit feed mass; oxidation changes the mass, so it must be measured

Worked example: the feed contains 25.0% sulphide sulphur and the oxidised residue 1.2%, and weighing shows the residue mass to be 84% of the feed mass. Sulphide oxidation is (25.0 − 1.2 × 0.84) ÷ 25.0 = 96.0%. Ignoring the mass change would give (25.0 − 1.2) ÷ 25.0 = 95.2%, understating the result.

Gold recovery after oxidation generally increases with sulphide oxidation, but the form of the relationship is specific to the ore. Some ores require nearly complete oxidation, while others release most of their gold well before that point. Testwork at several levels of oxidation sets the target, which in turn determines oxygen demand, residence time and cost.

Downstream processing

After oxidation, counter-current decantation thickeners wash the acid liquor from the solids. The solids are brought to leach pH with lime, and the acid liquor is neutralised with limestone and lime, a step that also fixes arsenic as stable ferric arsenate compounds where sufficient iron is present. The oxidised solids are then leached in CIL, as described in CIL circuit modelling. POX autoclaves recover heat from flash steam, whereas BIOX tanks require cooling water.

Glossary

Refractory gold
Gold that does not leach well with cyanide after normal grinding, usually because it is locked in sulphides.
Pressure oxidation (POX)
Oxidation of sulphides in an autoclave at high temperature and oxygen pressure.
Bio-oxidation (BIOX)
Oxidation of sulphides by bacteria in aerated tanks.
Autoclave
A sealed pressure vessel for reactions above the normal boiling point.
Sulphide oxidation
The percentage of sulphide sulphur converted to sulphate.
Basic iron sulphate
An iron sulphate compound that can form in the autoclave and consume lime and cyanide later.
Counter-current decantation (CCD)
A series of thickeners in which solids and wash water flow in opposite directions.
Neutralisation
Raising the pH of acid solids or liquor with limestone or lime.

Frequently asked questions

What makes a gold ore refractory?

Usually gold locked within sulphide minerals as particles too fine to liberate, or within their crystal structure. Carbonaceous matter that adsorbs gold (preg-robbing) is another cause.

How much oxygen does pressure oxidation require?

For pyrite fully oxidised to hematite and sulphuric acid, about 1.87 tonnes of oxygen per tonne of sulphide sulphur, plus an allowance for incomplete oxygen utilisation.

Is BIOX less expensive than POX?

It depends on scale, ore, power and site. BIOX operates at low temperature and pressure but requires several days of residence time and large tanks, while POX is faster but requires an autoclave and an oxygen plant. Studies compare both routes on the same ore.

Why must sulphide oxidation be corrected for mass change?

Because oxidation changes the mass of the solids. Comparing sulphur grades without the mass ratio gives an incorrect result.

Discuss your plant with a metallurgist

Tiegel is a Perth metallurgy company. We help with testwork, plant optimisation, metal accounting and investigations, and we build the Tiegel Suite software.

Talk to a metallurgist

References and further reading

  1. Marsden, J.O. and House, C.I. (2006). The Chemistry of Gold Extraction, 2nd edition. Society for Mining, Metallurgy and Exploration.
  2. Metso. Complete process and equipment solutions for refractory gold treatment. Link
  3. SGS Minerals (2009). Basic iron sulphate: a potential killer in the processing of refractory gold concentrates by pressure oxidation. Technical paper 2009-06. Link

Worked examples and charts marked illustrative use invented figures, not data from any operation.