Roasting refractory gold concentrates: two-stage roasting, sulphur dioxide and calcine

How roasting releases gold from sulphides and carbon: two-stage roasting for arsenic, oxygen, air and SO2 per tonne of sulphur, calcine mass and gas handling.

· 4 minute read · By

Roasting is the longest-established method of treating gold locked in sulphides. The concentrate is heated in air until the sulphides oxidise, the sulphur leaves as sulphur dioxide, and the iron forms a porous oxide in which the gold is accessible to cyanide. Roasting also burns organic carbon, which would otherwise adsorb dissolved gold during leaching. The main difficulty is the off-gas: sulphur dioxide and, in many ores, arsenic must be captured, so a modern roaster includes a substantial gas cleaning plant, usually with a sulphuric acid plant.

This article covers the chemistry of roasting, gas and air quantities, calcine mass and quality, and the two-stage process for arsenical ores. The alternative oxidation routes are covered in pressure oxidation and bio-oxidation.

Two-stage roasting of refractory gold concentrateStage 1 roasts with too little oxygen to drive off arsenic; stage 2 roasts with excess air to oxidise the remaining sulphur and carbon; the calcine is quenched and leached; the gas is cleaned, arsenic trioxide is collected and sulphur dioxide goes to an acid plant.ConcentrateStage 1 roasteroxygen-deficientStage 2 roasterexcess airQuench, thencyanide leachGas cleaning:dust, As₂O₃ collectedSO₂ toacid plantcalcinecalcinegas
A two-stage roasting circuit. Removing arsenic in the first stage under reducing conditions keeps it out of the calcine, where it would lower gold recovery.

Chemistry and gas quantities

4FeS2+11O2→2Fe2O3+8SO2mO2mS=1.37mSO₂mS=2.00mairmS=1.370.232=5.9

where

mO2mS
tonnes of oxygen per tonne of pyrite sulphur roasted, from 11 × 32.00 ÷ (8 × 32.06)
mSO₂mS
tonnes of sulphur dioxide per tonne of sulphur, from 64.07 ÷ 32.06
mairmS
tonnes of air with no excess; air is 23.2% oxygen by mass, and roasters run with excess air
Per tonne of pyrite sulphur roasted1.37 tonnes of oxygen, 2.00 tonnes of sulphur dioxide formed, and 5.9 tonnes of air with no excess.OxygenOxygen: 1.371.37Sulphur dioxideSulphur dioxide: 2.002.00Air, no excessAir, no excess: 5.925.92Tonnes per tonne of sulphur
Stoichiometric quantities for pyrite roasted to hematite. Every tonne of sulphur makes two tonnes of sulphur dioxide, which must be captured.

Worked example: 200 t/d of concentrate containing 30% sulphur, all as pyrite, contains 60 t/d of sulphur. Roasting produces 60 × 2.00 = 120 t/d of sulphur dioxide and requires 60 × 1.37 = 82 t/d of oxygen, or about 355 t/d of air with no excess. Roasters operate with excess air to complete the reactions, so the actual air flow is higher, with the excess set by design and operating experience.

Calcine mass and quality

Pyrite, FeS₂, loses mass on conversion to hematite, Fe₂O₃, each tonne of pyrite yielding about 0.67 t of hematite. In the example, 60 t/d of sulphur corresponds to 112 t/d of pyrite, which forms about 75 t/d of hematite. If the remaining 88 t/d of minerals pass through unchanged, the calcine is about 162 t/d, and the gold grade increases by a factor of about 1.23. The calcine is weighed and assayed to confirm this, because carbonates, arsenic minerals and other constituents also change mass.

Good calcine is porous. Roasting temperature and oxygen supply are controlled so that all sulphide and carbon is oxidised without overheating, since hot spots can partially melt or sinter the calcine and seal gold within iron oxide where cyanide cannot reach it. The calcine is quenched in water as it leaves the roaster and then leached, often after washing to remove soluble salts.

Two-stage roasting of arsenical ores

Arsenopyrite roasted in excess air can form arsenates that remain in the calcine and impair leaching. In a two-stage roaster, the first stage operates with a deficiency of oxygen, so that arsenic leaves as volatile arsenic trioxide while the iron sulphide is only partly roasted. The second stage, with excess air, completes the oxidation of sulphur and carbon. The arsenic trioxide is condensed from the cooled gas and collected for secure storage or sale.

Gas handling

Cyclones and hot electrostatic precipitators recover calcine dust, which carries gold, and return it to the process. Gas cooling condenses arsenic trioxide, which is captured in bag filters. Sulphur dioxide is converted to sulphuric acid in an acid plant or scrubbed, and the gas must remain above its dew point until it reaches the cleaning plant to avoid corrosion. Mercury and other volatile elements, where present, require their own capture steps and are identified in testwork.

Roasting compared with pressure oxidation

Roasting suits concentrates containing organic carbon, which pressure oxidation does not fully destroy, and sites where sulphuric acid can be sold. Pressure oxidation avoids sulphur dioxide and arsenic trioxide emissions and often gives higher gold recovery on pyritic ores. The choice is based on testwork on both routes, capital and operating costs, and the environmental approvals available at the site.

Glossary

Roasting
Heating a concentrate in air to oxidise sulphides and organic carbon.
Calcine
The solid product of roasting.
Two-stage roasting
A first stage short of oxygen to remove arsenic, then a second stage with excess air.
Arsenic trioxide
As₂O₃, the volatile arsenic compound driven off in the first roasting stage and collected from the gas.
Sintering
Partial melting and fusing of particles at high temperature, which can seal gold away from cyanide.
Excess air
Air supplied beyond the stoichiometric need, to complete the reactions.
Acid plant
A plant that converts sulphur dioxide into sulphuric acid.
Preg-robbing
Adsorption of dissolved gold by carbonaceous matter in the ore.

Frequently asked questions

How much sulphur dioxide does roasting produce?

About 2.0 tonnes per tonne of sulphur, from the molar masses of sulphur and sulphur dioxide.

Why roast in two stages?

To remove arsenic as volatile arsenic trioxide in the first, oxygen-deficient stage, so that it does not remain in the calcine as arsenate. The second stage completes the oxidation.

What temperature is used for roasting?

Vendor literature gives roughly 500 to 800 °C, depending on the process and mineralogy. The exact temperature is set by testwork and controlled closely to avoid sintering.

Does roasting treat preg-robbing carbon?

Yes. Roasting burns organic carbon, which is one of the reasons it is selected for carbonaceous refractory ores.

Discuss your plant with a metallurgist

Tiegel is a Perth metallurgy company. We help with testwork, plant optimisation, metal accounting and investigations, and we build the Tiegel Suite software.

Talk to a metallurgist

References and further reading

  1. Marsden, J.O. and House, C.I. (2006). The Chemistry of Gold Extraction, 2nd edition. Society for Mining, Metallurgy and Exploration.
  2. Metso. Complete process and equipment solutions for refractory gold treatment. Link
  3. Metso. Gold two-stage roasting. Link

Worked examples and charts marked illustrative use invented figures, not data from any operation.